MaterialsTechnical Article

ASTM A536 Ductile Iron:
Grades, Properties and Testing

ASTM A536 is the ASTM specification for ductile iron castings. Each grade number states three minimum properties, verified on test bars cast from the same iron. This article explains how to read the grades, how they compare with GB/T, EN and JIS designations, and what to state on a drawing.

Tensile test of a ductile iron test bar at Longtai

What ASTM A536 Covers

ASTM A536 covers castings in ductile iron, also known as spheroidal graphite (SG) or nodular iron: cast iron in which the graphite is substantially spheroidal. The graphite form is what separates it from gray iron; see Ductile Iron vs Gray Iron.

Tensile properties are the core requirement. Every grade sets a minimum tensile strength, yield strength and elongation. Hardness, chemical composition, microstructure, pressure tightness, radiographic or magnetic particle inspection, dimensions and surface finish apply only when the contract or purchase order calls for them.

How to Read a Grade Number

The three numbers in a grade are its minimums in inch-pound units. 65-45-12 means a tensile strength ≥ 65 ksi (448 MPa), a yield strength ≥ 45 ksi (310 MPa) and an elongation ≥ 12%. The specification treats inch-pound values as the standard; MPa values are conversions for information.

Grades and Minimum Properties

GradeMinimum tensile strengthMinimum yield strengthMinimum elongationUsual condition
60-40-1860 ksi (414 MPa)40 ksi (276 MPa)18%Ferritizing anneal
65-45-1265 ksi (448 MPa)45 ksi (310 MPa)12%As-cast
80-55-0680 ksi (552 MPa)55 ksi (379 MPa)6%As-cast
100-70-03100 ksi (689 MPa)70 ksi (483 MPa)3%Quench and temper, normalize and temper, or isothermal treatment
120-90-02120 ksi (827 MPa)90 ksi (621 MPa)2%Quench and temper, normalize and temper, or isothermal treatment
For special applications
60-42-1060 ksi (415 MPa)42 ksi (290 MPa)10%—
70-50-0570 ksi (485 MPa)50 ksi (345 MPa)5%—
80-60-0380 ksi (555 MPa)60 ksi (415 MPa)3%—
Minimum values per ASTM A536. Inch-pound values govern; MPa values are conversions for information. Yield strength is determined at 0.2% offset. The last three grades are listed separately for special applications such as pipe and fittings. Usual condition as summarized by ASTM; the drawing or purchase order may state otherwise.

Recent Longtai ductile iron shipments have been in 60-40-18, 65-45-12 and 80-60-03; other grades can be produced on request. See Materials and standards.

Choosing a Grade

Moving up the table trades elongation for strength. A practical rule is to specify the lowest grade that carries the design load, keeping elongation where shock or sudden fracture is a risk.

  • 60-40-18: the highest elongation and toughness of the general grades, for parts that see shock or must deform before cracking. In our catalog: the F-K pump diverter valve (84 kg) and valve body cover (28 kg).
  • 65-45-12: a balance of strength and elongation, and the grade of most slurry pump castings in our catalog, from the suction side casing (980 kg) and suction plate (159 kg) to the stuffing box (80 kg).
  • 80-55-06: higher strength where 6% elongation is sufficient, usually as-cast.
  • 100-70-03 and 120-90-02: strength reached through heat treatment, for parts where strength and wear resistance matter more than elongation. The specification cautions that quenched and tempered ductile iron may have substantially lower fatigue strength than as-cast material of the same hardness.
Ductile iron slurry pump suction plate, ASTM A536 65-45-12, 159 kg

How A536 Properties Are Verified

Tensile properties are measured on test bars machined from separately cast coupons, a Y-block, keel block or modified keel block, poured from the same ladle or heat as the castings and given the same heat treatment. If the purchaser states no preference, the manufacturer selects the coupon.

The specification also notes that no precise relationship can be stated between the properties at various locations in a casting and those of a test bar, as section size and cooling rate differ. If properties in the casting itself matter, state the requirement on the drawing or purchase order.

At Longtai, every heat is analyzed on a SPECTRO optical emission spectrometer (29+ elements) before pouring. Test bars are pulled on a 30 t tensile testing machine for tensile strength and elongation, hardness is checked in HB or HRC, and metallography confirms the graphite form. See Melting for how chemistry is controlled.

A536 Equivalents in GB/T, EN and JIS

USA · ASTM A536China · GB/T 1348Europe · EN 1563Japan · JIS G5502
60-40-18QT400-18EN-GJS-400-18FCD400-18
65-45-12QT450-10EN-GJS-450-10FCD450-10
80-60-03QT600-3EN-GJS-600-3FCD600-3
Approximate equivalents, for reference only. The standard on the drawing governs.

The equivalents are close but not identical, and the designations show it. QT450-10 and EN-GJS-450-10 call for 450 MPa and 10% elongation; 65-45-12 calls for 65 ksi (448 MPa) and 12%. QT400-18 calls for 400 MPa against 60 ksi (414 MPa) for 60-40-18. A casting certified to one standard is therefore not automatically compliant with another. Quote the governing standard on the drawing so that test bars are made and evaluated to it.

What to State on the Drawing or RFQ

  • Standard and grade, for example ASTM A536 65-45-12, with the edition if your quality system requires it.
  • Test coupon type, if you have a preference: Y-block, keel block or modified keel block.
  • Requirements beyond tensile properties, such as a hardness range, nodularity or microstructure, pressure tightness, or radiographic or magnetic particle inspection. A536 applies these only when the order calls for them.
  • Quantity and supply condition: as-cast, machined or painted.

Not sure which grade suits your part? Send your drawing for engineering review. We reply within 72 hours.